Vacuum System on a Pulp Carton Line: What Drifts and How to See It
Why does vacuum matter more than the mould?
On a pulp forming line the mould sets the shape, but vacuum sets how much fibre arrives on that shape. A mould can be perfect and still produce light, thin walls if the vacuum at the face has dropped.
That is why a carton that suddenly weighs less usually points at the vacuum line, not at the mould and not at the furnish.
Which vacuum readings should be logged each shift?
Three: the vacuum at the receiver tank, the vacuum at the forming head, and the time the head holds vacuum during the form. A single gauge at the pump tells you the pump is running, not that the mould face is seeing vacuum.
Log all three at the start and middle of each shift. A gradual fall across weeks is normal wear; a step change in one shift is a leak or a blocked line.
Where do leaks usually start?
At flex points rather than at joints. The hose that moves with the forming head fatigues first, then the swivel fittings, then the seals at the head. A leak at a moving part is also the hardest to hear, because the machine noise masks it.
Check the moving section first when vacuum falls and no blockage is found. A soap solution on the joints during a stop identifies most leaks in minutes.
How does vacuum change carton weight?
Weight scales roughly with the fibre deposited, which scales with vacuum within the working band. A five percent vacuum loss typically shows as two to four percent weight loss on the same mould and furnish.
That is small enough to pass a casual check and large enough to change compression strength by a measurable margin. Weigh ten cartons per shift and plot it against the vacuum log.
What is the maintenance interval for the vacuum side?
Filters and water separators need attention far more often than pumps. On a line running two shifts, inspect the separator weekly and the filter element on condition rather than on a fixed calendar.
Record the element change date on the machine. When vacuum problems recur, the log distinguishes a dirty site from a worn pump in one look.
How is a vacuum drop proved to be the cause rather than guessed?
Run a controlled pair: form ten cartons at the current setting, then ten at the previous known-good setting, and weigh both groups. If the weight difference matches the vacuum difference, the vacuum is the cause and the mould can be left alone.
Do it inside one shift and keep the cartons. A pair of weighed samples settles in ten minutes a question that otherwise runs for a week across shifts, and it gives the maintenance team a target instead of an opinion.
See also Mould Cavity Count Selection · Denesting Force on a Packing Line · Egg Carton Moisture: Oven-Dry Method · Furnish Blend and Forming Yield · Mould Cavity Balancing Guide · Closure Tab Interference on the Line.