A moulded logo reads when it sits 0.8 to 1.5 millimetres proud of the surface, carries a 0.4 to 1.0 millimetre edge radius, has at least 12 degrees of draft on every wall, and keeps 1.6 to 2.0 millimetres of wall thickness beneath it. Below 0.6 millimetres the relief fills with fines during forming and fades within two production runs. Depth alone does not make a mark; the wall under it and the screen above it decide whether it survives.
A Logo That Vanished in One Week
In spring a dairy co-operative in Jutland ordered 200,000 twelve-egg cartons with its name moulded into the lid, 0.5 millimetres in relief, replacing a printed logo it had used for four years. The artwork was approved from a single moulded sample that looked crisp under the office light.
By the second delivery the relief had almost gone. Operators could see the outline only at a low angle, and a retailer's quality team flagged the cartons as unbranded, holding 60,000 units at the depot.
The sample had been made on a freshly washed screen with a slow forming cycle. Production ran at 22 cycles per minute, and the shallow relief filled with fibre fines within 900 shots.
The tooling had a second problem. The 0.5 millimetre relief had been cut with 6 degrees of draft, which dragged fibre on release and left a torn fillet along one edge of the letters. Each tear held more fines, so the mark degraded faster on that side.
The co-operative re-cut the insert at 1.1 millimetres of relief with 14 degrees of draft, moved the mark from the lid curve to the flat centre panel, and added a screen wash every 400 shots. The mark held through 400,000 cartons with a legibility check at each shift.
How Relief Is Formed
An embossed mark is a negative in the forming tool. The tool carries a recessed pocket, a fine screen is stretched over it, and vacuum pulls fibre into the pocket during the forming stroke, so the pocket fills with pulp and the carton comes out with a raised mark.
Three things determine how much fibre lands there. The screen mesh: a finer mesh on the pocket holds shorter fibre and gives a sharper edge, but blinds faster. The vacuum duration, usually 0.6 to 1.2 seconds on a reciprocating machine; too short and the pocket fills only partly, too long and the whole wall thickens. And the furnish: a blend with 20 to 30 percent longer fibre holds a relief edge better than a fines-heavy recycled furnish.
Because the mark is formed, not pressed, it cannot be added after the fact. Depth must be in the tool, and so must its draft.
Wall Thickness Under the Relief
A relief borrows fibre from the wall beneath it. Thickening a mark on the outside thins the wall on the inside, so a 1.5 millimetre relief on a 1.6 millimetre wall produces a weak spot directly under the logo, and that is where the lid cracks after a few hundred kilometres.
Keep the residual wall at 1.6 to 2.0 millimetres and the relief at no more than 35 to 40 percent of the nominal wall. Measure it by cutting a section through the mark and reading thickness with a micrometer, a check that takes ten minutes and prevents a recurring failure.
| Relief depth | Draft used | What happens over a run | Legibility at 400 mm |
|---|---|---|---|
| 0.3 to 0.5 mm | 5 to 8 degrees | Fills with fines within 500 to 1,500 shots | Fades to a shadow |
| 0.6 to 0.7 mm | 8 to 10 degrees | Partial fill, edge tears at release | Reads only at a low angle |
| 0.8 to 1.0 mm | 10 to 12 degrees | Stable, mild fill on the upwind edge | Reads in normal light |
| 1.1 to 1.3 mm | 12 to 15 degrees | Stable for 300,000 plus shots | Sharp, reads at arm's length |
| 1.4 to 1.5 mm | 15 degrees | Stable if wall is 2.0 mm or more | Sharp, strong shadow line |
| over 1.6 mm | 15 degrees plus | Wall thins, lid cracks under stack load | Sharp but structurally costly |
Draft and Release
Every wall of the pocket needs draft, or the carton tears as it leaves the tool. Twelve degrees is the practical floor on a 1 millimetre relief; fifteen is comfortable, and twenty is used on deep marks where release speed is high.
Draft is measured on the vertical face of the letter stroke, and the number people quote is often the angle of the whole pocket rather than of the stroke. A serif or a tight curve has a face that is nearly vertical even when the pocket looks drafted, and that is where tears start.
Tears are not only cosmetic. A torn fillet is a fibre trap, and a fibre trap blinds within a few hundred shots. If the first samples show a rough edge on one side of the letters, the answer is draft, not a longer forming time. Where a letter has a sharp internal corner, add a 0.5 millimetre radius before adding degrees of draft, because the radius does more for release than three extra degrees.
Where the Mark Should Sit
Put the mark on the flattest area available, usually the centre of the lid panel. The transition where the lid curves into the side wall stretches the screen locally, and a mark there prints at 60 to 80 percent of its intended depth.
Keep 8 to 10 millimetres clear of the hinge, because the hinge needs full wall thickness and the score line needs an uninterrupted surface. Keep 5 millimetres clear of any cup rim, since the rim is a load path.
Design copy for forming, not for print. A stroke width under 0.8 millimetres fills in, counters smaller than 1.2 millimetres close up, and letter heights under 4 millimetres lose their shape. Two or three words read better than a sentence; a mark that needs a magnifier in the sample will be invisible in a cold store. Walk the artwork past the toolmaker before the pocket is cut, because a mark that cannot be formed is far cheaper to redraw than to re-cut.
Screen Blinding and Cleaning
Fines are the enemy of a moulded mark. Every forming cycle passes short fibre and fines across the screen, and a recessed pocket catches them preferentially because the flow there is slower.
Wash the pocket on a fixed count, not when the mark looks bad. On a fast line, 300 to 500 shots is a working interval; on a slow line with a long vacuum, 800 to 1,200 can be safe. The interval should be set by legibility checks, not by the calendar.
Record the wash count with the carton count. When the mark fades, the first question is how many shots since the last wash, and a supplier who cannot answer it is guessing.
ISO 534 sets the method for measuring the thickness of paper and board, and a section through an embossed mark is measured exactly that way before the relief is approved.
Where the same lid carries print, the print area plan must leave the embossed panel free, and the draft angle rules for deep cavities apply to letters as much as to cups. If the mark sits near a cup, the wall thickness check comes first, because a logo is never worth a cracked lid. Where a moulded mark is weighed against a printed one, the printing and branding options comparison sets cost and life side by side, and the shape consistency audit shows how much a mark contributes to the impression a customer actually forms.
Proving Legibility Before Tooling
Approve a mark at arm's length in the lighting where it will be seen: 400 millimetres away, 500 lux, on three cartons from the same shot, with two people judging independently. A single sample under office light is how the Jutland logo was approved.
Then approve a second sample after 400 shots without a wash. That is the state the customer will see for most of the run, and a mark that only reads when the screen is fresh has not been proven.
Commission the tool only after both samples pass. Re-cutting a pocket costs 800 to 2,500 euros and four to six weeks, which is more than the entire branding budget on a mid-size order.
Relief depths, draft angles and shot counts here come from tooling drawings, forming trials and packer legibility checks rather than from a moulded packaging standard. Fibre blend, machine speed and screen mesh will move the window, so treat the table as a tested band rather than a fixed rule.
Related reading
AI Assistance Disclosure
Relief depths, draft angles and shot counts here come from tooling drawings, forming trials and packer legibility checks rather than from one moulded packaging standard. Fibre blend, machine speed and screen mesh will shift the window, so the bands are measured starting points rather than fixed rules.